Research Theme · 02

Corrosion-Induced
Deterioration

Airborne chloride-ions penetrates the concrete cover of structures and turns the steel into rust. The process is modeled as non-uniform pitting, cracked cover, weakened columns and joints, and follow it all the way to how the frame will behave in an earthquake.

Based on our 2026 paper in the Journal of Building Engineering.

A DETAIL A · 2.6× SCHEMATIC COLUMN SECTION
0years
As built
The concrete cover keeps the steel passive.
fig. 2.0Drag the slider to age the column. The ties sit under 32 mm of cover and the main bars under 40 mm; the mean start of corrosion (17 and 20 years) and the 50-year bar loss come from the study. The timing of cracking and spalling is drawn schematically.
Sheet 1Context & motivation

A slow hazard on top of a sudden one

Much of the RC building stock in India's seismically active coastal belts was designed for gravity loads alone, so these frames start out with little ductility. Then wind-borne chlorides go to work: in coastal areas most deterioration comes from corrosion, and it attacks the very steel the frame needs to survive an earthquake.

Two weaknesses that compound Left: a column and beam–column joint with widely spaced ties and no ties in the joint. Middle: a reinforcing bar in cracked cover concrete, with pits along its length. Right: seismic capacity over the service life — a pre-code frame starts below a code-conforming frame and keeps losing capacity once corrosion starts. Low-ductility detailing built in from day one widely spaced ties no ties in the joint shear-critical column + Corrosion added year after year cover cracks spalls deep pits chlorides diffuse in from the surface = Compounded over time seismic capacity over the years (schematic) capacity 0 20 50 yr code-conforming frame pre-code frame less ductile from day one lost to corrosion
fig. 2.1Two weaknesses that compound: deficient detailing sets a low starting point, and corrosion keeps taking capacity away once it starts. In coastal areas, 70–90% of deterioration comes from corrosion.

What existing assessments miss

Corrosion isn't uniform

Most models reduce rebar cross-sectional area evenly. Realistic corrosion is often pitted, and it varies along each bar and over time.

Shear limits ignore corrosion

Drift-based shear limits don't consider the shear strength a corroded column has lost.

Joints are left out

Beam–column joint deterioration is routinely omitted, though joints often govern failure in low-ductility frames.

Damage seen column by column

Damage limit states that track columns alone under-represent what happens to the frame as a system.

Sheet 2Methodology

From corrosion initiation to time-dependent fragility

The model follows deterioration from the material up to the whole frame: when corrosion starts, how fast it runs once the cover cracks, how pits spread along each bar, what that does to concrete, steel, columns and joints — and finally how the ageing frame responds to earthquakes typical of the region.

Case study: a three-bay, three-storey low-rise RC frame representative of the region.

01

Corrosion starts

Monte Carlo simulation: ties first (mean ≈ 17 years), main bars at ≈ 20 years.

02

Cover Cracking

A corrosion rate that jumps once the cover cracks, scaled by initial and severe cracks.

03

Pits along every bar

Pit depth varies along the bar: defined as a lognormal pitting factor.

04

Secondary losses

Mass loss weakens the concrete, the steel, and the shear strength of columns and joints.

05

Frame model

OpenSees frame with fibre sections, shear and rotational springs for column and joint responses.

06

Damage & fragility

Component damage mapped to global response, compared with demand from region-specific records.

Corrosion rate after initiation, with and without the effect of cover cracking (schematic). 20 50 Exposure age (years) Corrosion rate cover cracks with cracking effects without cracking
fig. 2.2Once the cover cracks, the corrosion rate jumps and then decays only slowly. The self-accelerating effect that uniform-rate models miss.
Three bar cross-sections: uniform corrosion, a pit, and both together. Uniform even reduction Pitting localized pits Both what real bars face original bar rust-filled pit
fig. 2.3Uniform corrosion thins the whole bar; a pit takes a deep local bite. Together they remove far more of the bar's area.
Bars simulated: 0
(the study ran 2,000)
fig. 2.4Pits are not the same depth along a bar. The study draws the pit depth of each segment from a lognormal pitting factor and carries the median into the frame model. Drawn here with illustrative values.
The frame model A three-bay, three-storey frame. Columns are fibre-section elements with shear springs at their ends, beams have plastic hinge zones at both ends, and each beam–column joint is a rotational spring inside rigid links. Insets show a fibre section and a joint spring backbone before and after corrosion. a b Columns: nonlinearbeamcolumnelements, fibre sections Beams: beamwithhinges elements Joints: rotational springs, rigid links Column ends: shear springs for shear failure a · fibre section cover (unconfined) core (confined) steel layers Corrosion lowers fc, fy and the steel area. b · joint spring uncorroded corroded rotation moment
fig. 2.5The frame is modeled in OpenSees. Corrosion enters through the fibre materials and the spring backbones.
Sheet 3Outcomes

What fifty years of corrosion does to a frame

What remains at 50 years Lost
Share of each property remaining after 50 years. Rebar area: up to 47% lost. Cover concrete strength 89% lost, rebar ductility 76%, joint shear strength 36%, column shear strength 26%, rebar yield strength 24%. DRIVER Rebar area (pitting) up to −47% KNOCK-ON LOSSES Cover concrete strength −89% Rebar ductility −76% Joint shear strength −36% Column shear strength −26% Rebar yield strength −24%
fig. 2.6Losses at 50 years relative to the as-built frame. Degradation models: Biondini and Vergani (2015) for cover concrete and ductility, Zhang and Li for joints, Vu et al. (2016) for column shear, Du et al. (2005) for yield strength.

The losses are far from even

Pits take up to 47% of a bar's area where they concentrate. The knock-on damage is uneven: the cover concrete is almost gone, the steel loses most of its ability to stretch before breaking, and the joints lose more shear strength than the columns.

As built After 50 years Damage states S · M · E · C
Schematic capacity curves: the 50-year frame peaks at less than half the as-built base shear and reaches each damage state at a smaller drift. Maximum inter-storey drift Base shear SMEC SMEC −56% peak base shear damage states arrive sooner
fig. 2.7Capacity curves from pushover analysis, drawn schematically. Damage-state points (S slight, M moderate, E extensive, C complete) arrive at smaller drifts after deterioration.

More than half the lateral strength is lost

After 50 years of coastal exposure the frame's base-shear capacity falls by more than half, and every damage state is reached at a smaller drift, the frame is both weaker and less able to deform before it is damaged.

Smaller earthquakes do the same damage

A fragility curve gives the probability of reaching a damage state at a given shaking intensity. After 50 years every curve shifts left, the heavier the damage, the bigger the shift, and the curves flatten, so the aged frame is both weaker and less predictable. Pick a damage state to compare the curves.

Median intensity to reach each damage state
as built  →  after 50 years
As built 50 years
Show the numbers
Damage stateAs built median (g)Dispersion50-year median (g)DispersionChange in median
Slight0.390.380.260.51−33%
Moderate0.790.390.480.54−39%
Extensive1.060.400.590.54−44%
Complete1.470.430.720.55−51%
fig. 2.8Fragility curves with the medians and dispersions from the study; intensity is the average spectral acceleration. Hover the chart, or focus it and use the arrow keys, to read probabilities.
Left: an as-built column with flexural cracks near its ends. Middle: a corroded column with a diagonal shear crack. Right: a beam–column joint with diagonal cracks. hinge As built flexural failure shear crack After 50 years fails in flexure–shear Joint shear cracking in the panel
fig. 2.9How the governing failure changes with corrosion (schematic).

Columns fail differently, joints matter

Non-uniform pitting shifts the columns from flexural to flexure–shear failure at times, which is more brittle. Leaving joint deterioration out of the model gives an inaccurate picture of how the ageing frame actually fails.

Put together, spatially varying non-uniform corrosion, joint deterioration and region-specific ground motions, the framework gives a more realistic seismic risk estimate for low-ductility frames in corrosive environments.

Sheet 4Open for collaboration

Questions I'd like to work on with others

These are the threads I think are worth pulling next. If you work on any of them, in a lab, in the field or on a code committee, I would be glad to collaborate.

Corroded joints under cyclic load

Joint deterioration models still rest on few tests. Cyclic tests on corroded beam–column joints would sharpen them and the damage states built on them.

Good fit for: experimental labs with accelerated-corrosion set-ups.

Field data from coastal buildings

Chloride profiles, cover depths and measured mass loss from real buildings, ideally from non-destructive testing, would anchor the pitting model to what is out there, and let us forecast how fast each building is ageing.

Good fit for: inspection agencies, asset owners, NDT specialists.

A changing climate

Warmer, wetter conditions change corrosion rates. Coupling climate projections with time-dependent fragility could show which buildings will age fastest, and when to step in.

Good fit for: climate and durability researchers.

Beyond the 2D frame

Bond–slip between rusting bars and concrete, irregular 3D buildings, and combining with soil-structure interaction are still open.

Good fit for: modelling groups and durability researchers.

Working on something related? I'd be glad to hear from you.

PapersFrom this theme
Journal · 2026
Seismic damage limit states and fragility of low-ductility RC frames considering non-uniform corrosion and joint deterioration
Journal of Building Engineering, 115191
View paper ↗
Conference · 2024
Seismic damage limit states for aged reinforced concrete frame considering improved corrosion model
18th World Conference on Earthquake Engineering (18WCEE), Milan